Grau | ISO Grau | Composição Química(% em peso) | Características do pó | propriedades físicas como a poroso | ||||||||||
WC | Co | TiC | TaC | othe | T.C | Lubrificante | Média tamanho de grãoWC(um) |
Densidade Aparente g/cm3 | Fluxo taxa Sec/50g |
Hadrdness HRA±0.5 | Densidade g/cm3±0.1 |
TRS Mpa min |
||
CTF40D | - | 88.0 | 12.0 | - | - | - | 5.32 | 2.0%wax | 6.0 | 3.20 | 27 | 87.5 | 14.30 | 2800 |
CTD20A | - | 91.0 | 9.0 | - | - | - | 5.56 | 2.0%PEG | 8.0 | 3.70 | 25 | 86.5 | 14.60 | 2500 |
CTT20A | P20 | 79.3 | 8.0 | 8.7 | 4.0 | - | 6.82 | 2.0%wax | 2.0 | 2.70 | 30 | 91.8 | 12.40 | 2200 |
CTK10F | K10 | 93.3 | 6.5 | - | - | 0.20 | 5.76 | 2.0%wax | 1.8 | 3.40 | 27 | 92.0 | 14.86 | 3200 |
CTK30F | K30 | 91.1 | 8.5 | - | - | 0.4 | 5.63 | 2.0%wax | 1.8 | 3.10 | 29 | 91.0 | 14.65 | 2800 |
CTK50 | K50 | 90.0 | 10.0 | - | - | - | 5.52 | 2.0%wax | 1.8 | 3.20 | 28 | 90.5 | 14.54 | 2800 |
CTF05 | K02 | 97.0 | 3.0 | - | - | - | 5.98 | 2.0%wax | 4.0 | 3.35 | 25 | 92.0 | 15.25 | 2100 |
CTD22 | - | 90.8 | 9.2 | - | - | - | 5.55 | 2.0%wax | 4.0 | 3.20 | 28 | 88.4 | 14.62 | 2600 |
CTU15F | K10-K30 | 91.4 | 8.0 | - | - | 0.6 | 5.76 | 2.0%wax | 0.6 | 3.00 | 28 | 93.0 | 14.65 | 4200 |
CTU25UF | K10-K50 | 86.0 | 12.0 | - | - | 1.4 | 5.49 | 2.0%wax | 0.4 | 2.70 | 30 | 93.0 | 14.10 | 4000 |
CTU10 | K10 | 93.85 | 6.0 | - | - | 0.15 | 5.84 | 2.0%wax | 0.8 | 3.05 | 27 | 93.0 | 14.85 | 2700 |
CTU20 | K10-K20 | 89.5 | 10.0 | - | - | 0.5 | 5.57 | 2.0%wax | 0.8 | 2.85 | 30 | 91.8 | 14.45 | 3400 |
CTU30 | K20-K30 | 85.7 | 13.5 | - | - | 0.8 | 5.38 | 2.0%wax | 0.8 | 2.70 | 32 | 90.5 | 14.00 | 3500 |
CTK02 | K01 | 95.9 | 4.0 | - | - | 0.1 | 5.92 | 2.0%wax | 1.3 | 3.40 | 24 | 92.7 | 15.15 | 2100 |
CTK05 | K05 | 94.0 | 6.0 | - | - | - | 5.79 | 2.0%wax | 1.5 | 3.40 | 24 | 92.0 | 14.90 | 2450 |
CTK10 | K10 | 94.0 | 6.0 | - | - | - | 5.78 | 2.0%wax | 2.0 | 3.40 | 26 | 91.5 | 14.90 | 2500 |
CTK20 | K20 | 94.0 | 6.0 | - | - | - | 5.79 | 2.0%wax | 3.0 | 3.40 | 27 | 91.0 | 14.90 | 2600 |
CTK30 | K30 | 92.0 | 8.0 | - | - | - | 5.64 | 2.0%wax | 3.0 | 3.35 | 28 | 90.0 | 14.70 | 2700 |
CTK40 | K40 | 91.0 | 9.0 | - | - | - | 5.57 | 2.0%wax | 3.0 | 3.20 | 29 | 89.5 | 14.60 | 2800 |
CTF20D | - | 94.0 | 6.0 | - | - | - | 5.76 | 2.0%wax | 4.0 | 3.40 | 26 | 90.0 | 14.90 | 2600 |
CTF25D | - | 92.0 | 8.0 | - | - | - | 5.63 | 2.0%wax | 5.0 | 3.40 | 26 | 89.5 | 14.70 | 2800 |
CTF31 | - | 90.5 | 9.5 | - | - | - | 5.59 | 2.0%wax | 4.0 | 3.30 | 26 | 89 | 14.43 | 2800 |
CTF40 | - | 88.0 | 12.0 | - | - | - | 5.40 | 2.0%wax | 2.0 | 3.10 | 27 | 89.0 | 14.40 | 3000 |
CTF45 | - | 87.0 | 13.0 | - | - | - | 5.34 | 2.0%wax | 2.5 | 3.05 | 30 | 88.5 | 14.20 | 3100 |
CTF50 | - | 85.0 | 15.0 | - | - | - | 5.20 | 2.0%wax | 3.5 | 2.90 | 30 | 87.5 | 14.00 | 3000 |
CTF60 | - | 80.0 | 20.0 | - | - | - | 4.91 | 2.0%wax | 5.5 | 2.75 | 32 | 84.5 | 13.65 | 2700 |
CTF65 | - | 78.0 | 22.0 | - | - | - | 4.78 | 2.0%wax | 5.5 | 2.70 | 33 | 84.0 | 13.40 | 2700 |
CTF70 | - | 75.0 | 25.0 | - | - | - | 4.60 | 2.0%wax | 5.5 | 2.65 | 33 | 82.5 | 13.18 | 2400 |
CTD10 | - | 94.0 | 6.0 | - | - | - | 5.77 | 2.0%wax | 8.0 | 3.40 | 26 | 89.0 | 14.95 | 2500 |
CTD20 | - | 92.0 | 8.0 | - | - | - | 5.64 | 2.0%wax | 8.0 | 3.40 | 26 | 86.5 | 14.60 | 2500 |
CTD25A | - | 90.0 | 10.0 | - | - | - | 5.51 | 2.0%wax | 3.0 | 3.30 | 26 | 88.5 | 14.50 | 2850 |
CTD50 | - | 85.0 | 15.0 | - | - | - | 5.20 | 2.0%wax | 6.0 | 3.20 | 27 | 86.0 | 14.00 | 3000 |
CTT20 | P20 | 72.0 | 8.0 | 8.0 | 12.0 | - | 6.86 | 2.0%wax | 2.0 | 2.70 | 30 | 92.2 | 12.40 | 1900 |
CTT30 | P30 | 75.8 | 8.0 | 6.2 | 10.0 | - | 6.60 | 2.0%wax | 2.0 | 2.80 | 28 | 91.5 | 12.80 | 2100 |
Chinatungsten online produz vários tipos de pós para prensagem, que é amplamente utilizado na fabricação de produtos carbide.The cimentadas têm as seguintes características:
1、Estável Densidade aparente.
2、Graças à fluidez Excellen aspecto esférico do pó.
3、Bom compressibilidade.
4、Alta Pureza química, bem controle do teor de carbono.
5、O metal duro feito da nossa RTP tem excelentes propriedades físicas.